配方类型: |
RUBBER, PLASTICS, WAXES |
配方说明: |
Diethylene Glycol Maleate Polyester |
配方组成: |
In a 250-cc distilling flask, set for downward distillation and fitted with a thermometer and a gas-bubbling tube---both extending nearly to the bottom of the flask-plac Maleic Anhydride/88 g Redistilled Diethylene Glycol/106 g |
配制方法: |
Bubble in deoxygenated nitrogen until the air in the flask is displaced by nitrogen. Heat the flask and reaction mixture at 210 to 220'C over a wire gauze and hold at this temperature for two to four hours. Allow the mixture to cool, with nitrogen still passing into the system. The result should be a light-yellow, viscous liquid diethylene glycol maleate. Mix this compound with 10 to 30% of monomeric styrene and substitute this mixture for the polyesters used in the following formulas. |
|