    配方说明: Low density Nonshrinking Foamed Urethane
    配方组成: *diethylethanolamine/42
    HCl (36.5%)/24
    Distilled Water/34
    Adjust pH to 9.8
    Charge the castor polyol into a three-neck, one-liter flask fitted
    with a stirrer, thermometer and condenser with drying tube attached.
    Slowly add the tolylene diisocyanate to the charge with moderate
    agitation over a thirty minute period. then heat the reactants to the
    prescribed temperature for one hour. Cool to 65'C. and package in 1 qt.
    tinned cans.
    Foam Formulation Formul
    "Flexricin" 20/311
    Water Content 49.1%
    "Flexricin" 9/-
    DB Castor Oil/-
    Tolylene Diisocyanate 80/20/289
    Prepolymer/100.0
    Reaction Temperature/130'C
    Dimethyl siloxane "Dow-Corning" DC-200/.5
    "Flexricin" 15/-
    Buffered Diethylethanolamine*/4.4
    Distilled Water/.8
    "Estynox" 300/-
    配制方法: Laboratory Procedure for Foam Preparation: The dimethyl siloxane is hand mixed into the prepolymer. To this mixture is added the buffered diethylethanolamine together with the water. The blend is manually mixed to a point where incipient foaming becomes observable (about 45 seconds) after which it is poured into a waxed paper container to foam. The foam is allowed to cure at room temperature.