配方类型: |
EMULSIONS AND OTHER COLLOIDS |
配方说明: |
"Armowax" Emulsion |
配方组成: |
Glacial Acetic Acid/0.6 "Armowax"/20.0 Water/76.0 "Ethomeen" 18/12/3.4 |
配制方法: |
Heat the "Armowax" and "Ethomeen" to approximately 140'C. (284'F.). Add this mixture in a thin stream to the water and acetic acid heated to approximately 100'C. (212'F.), using vigorous agitation. continue stirring until smooth. for maximum fineness of particle size, use a colloid mill or equivalent. Lumping in the initial stage is a natural occurrence and will thin out on continued agitation. |
|