POLISHES |
配方说明: |
Floor Polish |
配方组成: |
Diethylethanolamine/2.5 Ammonium Hydroxide (26 C Be)/6.0 Tributoxy Ethyl Phosphate/0.5 by vol. Melt the wax and fatty acid together and adjust the temperature to 124'C. Add the amine to the melt with stirring and continue stirring until the melt is clear. Pour the melt slowly into water at 95-97'C under good agitation. As soon as emulsification is completed, cool the emulsion rapidly to 45'C and dilute to 15% N.V. with more water. Polish formula Formalin (37%)/0.15 "FC"-128 (1% sol'n.)/1.0 by vol. Water (hot)/224.0 Water (cold)/398.0 Tall Oil Fatty Acid/5.0 "Epolene" E-10/40.0 Diethylaminoethanol/5.0 Water/150.0 Diethylene Glycol Monomethyl Ether/7.39 "Polyrich" 10-N-30/2.12 "Epolene" Emulsion (above)/35.0 "Ubatol" U-3400/53.0 Tributoxyethyl Phosphate/2.20 "SMA" 2625 A (15% wt. sol'n.)/12.0 Ethylene Glycol/1.5 "Kodaflex" TXIB/0.7 Tributoxy Ethyl Phosphate/0.6 Formalin/0.14 2- |
|