生意宝 | 全球化工网 | 韩国化工网 | ChinaChemNet·免费注册 ·用户登录 ·服务中心 
  • 中国化工网首页 >> 化工助手 >> 化学配方数据库



    配方类型: POLISHES
    配方说明: Furniture Polish
    配方组成: Paraffin Wax/2.5
    Mineral Spirits/20.0
    1. Prepare 20% "Petrolite" C-36
    C: "Viscasil" (10,000)/3.00
    "Span" 60/1.5
    Mineral Spirits/3.39
    "Tween" 60/1.5
    B: "Carbopol" 934/0.2
    Sodium Hydroxide (10% sol'n.)/0.8
    Water/67.0
    Silicone Fluid "SF"-96 (350)/3.00
    A: Carnauba Wax (#1 yellow)/0.220
    Oleic Acid/5.20
    Beeswax/0.68
    "Tween" 80/0.066
    Mineral Spirits/6.90
    Water/1.914
    B: "Dow Corning" 922A Emulsion/7.200
    D: "Carbopol" 934 (1% dispersion in water)/3.50
    Oleic Acid/0.45
    Water/80.400
    C: "Carbopol" 934 (2% dispersion in water)/10.000
    Triethanolamine (1% sol'n. in water)/27.90
    D: Morpholine/0.200
    Morpholine/27.90
    E: Propellant/as required
    A: "G.E" SM-2133 Emulsion/4.0
    "G.E" SM-2135 Emulsion/2.0
    "Petrolite" C-36 (20%)/2.0
    B: "Carbopol" 934/0.20
    Triethanolamine/0.20
    B: Morpholine/0.23
    Water/91.25
    "Titanox" 3328/0.20
    A: Silicone Fluid "SF"-96/4.0
    Formali
    配制方法: Melt the wax and with mild stirring, bring temperature to 99 C (210 F). Add the oleic acid with stirring and when thoroughly mixed, add the morpholine. Slowly add the water, preheated to 99'C (210'F), to the wax/soap mixture maintaining the temperature at 93-99'C (200-210'F) until all the water has been added. Continue stirring until the temperature reaches 43'C (110'F). Then cool to room temperature.
    2. Blend Part A and Part B components separately.
    3. Add Part A slowly to Part B with mild agitation. Continue agitation until a homogeneous mixture is obtained.
    Note: Distilled or demineralized water is preferable.