    配方类型: EMULSIONS
    配方说明: Thickening Elastomer Latex
    配方组成: Water/66.0
    "Carbopol" 934/2.8
    "Geon" Vinyl 576 (55% total solids)/182.0
    sodium hydroxide (10% solution)/8.9
    配制方法: 1. Disperse the "Carbopol" 934 in water. This can be done best with moderate or high-shear mixing.
    2. Neutralize the "Carbopol" 934. In all cases "Carbopol" resins must be neutralized with a base such as sodium or ammonium hydroxide to develop their unique properties. After the acid solution has stood long enough to release air bubbles, neutralize the acid "Carbopol" dispersion to pH 7 to 9 by slowly adding the desired base with mild agitation. This can be done by using from 4.2 to 5.1 pounds of a 10% solution of sodium hydroxide per pound of "Carbopol" resin. A heavy water gel will form.
    3. Add the latex to the preneutralized "Carbopol" solution with moderate agitation. It is very important that the latex be added to the preneutralized "Carbopol" solution rather than the reverse. By adding the latex to the preneutralized "Carbopol" gel, uniform dispersion of the gel is insured. The first portion of the latex must be added very slowly. Addition of latex too rapidly will break the "Carbopol" gel into

    返回数据库查询
    其他库:化学品法规 国家标准 化学品安全数据库(msds) 外贸常识 合同范本 报关指南 商检指南 国际区号 国家代码