配方类型: |
METALS AND THEIR TREATMENT |
配方说明: |
Coloring Copper Blue |
配方组成: |
Gelatin/0.5 oz/gal Cathode current density/1.5 to 4 A/ft^2 Copper acetate/1.5 oz/gal Formula No. Sodium thiosulfate/8 oz/gal Lead acetate/4 oz/gal Temperature/200'F Immersion time/30 to 60 sec. |
配制方法: |
At temperatures below about 170'F, thin yellow, green, or red films are obtained, depending on the immersion time. With an addition of potassium. |
|