    配方类型: RUBBER, PLASTICS, WAXES
    配方说明: Polyester Premix Molding
    配方组成: "Asp"-400 (clay)/35
    tert-Butyl peroctoate/1.0% based on P19A
    Asbestos 7T-15/5
    "Zelec" UN/0.5% based on P19A
    "Paraplex" P19A (60 parts P340/40 parts P543)/35
    -in H.S.I. glass fibers/25
    配制方法: Alternate catalysts: tert-Butyl perbenzoate, benzoyl peroxide.
    Mixing times: 2 min for resin and fillers, 3 min after addition of glass. "Zelec" UN is the recommended release agent. Apart from these components, the formulation may be modified as desired to produce optimum-quality parts. After the formulation has been mixed, parts should be molded promptly. If there is to be a delay before molding, the material should be wrapped in cellophane, polyethylene film, or wax paper.