    配方类型: CEMENT & CERAMICS
    配方说明: Metal Preparation for Low Temp. Vitreous coating
    配制方法: Steel Pickling Method: 1. Cleaner bath 13/3 oz./gal. Wyandotte W.L.G. cleaner, (or equiv.), boiling 20 min.
    2. Water-rinse-room temperature 3. Acid 6-8% sulfuric acid, 150'F./10 min.
    4. Water rinse---room temperature 5. Nickel dip 1 oz. single nickel salts/gal., pH 3.2-3.5, 160'F. /10 min. (sufficient to get 0.06-0.08 gm. nickel) (sq. ft.) 6. Water rinse---room temperature 7. Neutralizer. 16 oz./gal. sodium carbonate, .05 oz./gal. borax, 155-175'F/2-3 min.
    8. Neutralizer using 1/4 avove strength 9. Dryer Aluminized steel Method A 1. Diversey # 404 cleaner 8 oz./gal., 170'F./2 min.
    2. Spray rinse (cold) 3. 7% H2SO4, 140-150'F./2 min.
    4. Spray rinse (cold) 5. neutralized (weak) 1 oz. borax/gal., 1/4 oz. soda ash/gal., 1-2 min.
    170'F.
    6. spray rinse (cold) deionized water 7. Hot rinse (optional) 8. Quick dry Method B Preheat metal at 1000'F./10 min.
    Method C 1. Vapor degreasing 2. Hot rinse 3. Dry Method D Organic solvent cleaner Miscellaneous Sandblasting is preferred for