配方类型: |
INKS |
配方说明: |
Fluorescent Letterpress and Litho Ink |
配方组成: |
Drain. Wax Compound**/12.0 **25% AC #6 polyethylene wax in Inkol O solvent. Heat solvent to 110'C, add wax, cool with stirring. 12% Cobalt Drier/0.3 Pigment, FH and/or F-S-Series/44.8 Eugenol Compound/0.3 Vehicle*/41.7 *50% Pentalyn G in China Wood Oil. heat oil and resin to 200'C and Lead-Manganese Drier (Pb 11%---Mn %)/0.9 |
配制方法: |
Add vehicle, wax compound and pigment in order and pony mix. Three-roll mill with first pass semi-tight and subsequent passes tight. All passes run slow speed. After grind is satisfactory, add driers and eugenol and loose pass on mill, When desirable, a solvent such as Inkol O may be used to reduce tack. |
|