配方类型: |
RUBBER, PLASTICS, WAXES |
配方说明: |
Humid Aging Characteristics of "PAPI" Foams |
配方组成: |
$G: "Pluracol" PEP-450 "QUADROL" "Quadrol"/as shown below "PAPI" Triethylamine/1.0 Rise time (min-sec) Density before aging (pcf) Volume change (%) Weight change (%) Density after aging "Dow Corning" 113/3.0 (pcf) Fluorocarbon 11/60.0 Compressive strength After aging psi at 7.5% deflection "Pluracol" PEP-450/as shown below "PAPI"/as shown Tetramethylguanidine/3.0 |
配制方法: |
With the resin system shown, using "Pluracol" PEP-450, increasing the amount of "Quadrol" will improve the humid aging characteristics of the resulting foam. The volume swell after exposure for seven days at 100% relative humidity at 158'F will decrease from 15.4 to 0% as the amount of "Quadrol" is increased from 0% to 40% by weight, and the final strength of the foam will be slightly increased. The content of closed cells and probably retention of the "K" factor are improved with 20% to 30% "Quadrol." |
|