中国化工网首页 >> 化工助手 >> 化学配方数据库
配方类型: |
POLISHES, ABRASIVES |
配方说明: |
Buffing & Polishing Media (Color Liquid Formulation) |
配方组成: |
TRITON X-100/0.13 TO 0.50 Loading Levels % TRIPOLI R-15/40.0 TO 50.0 Loading Levels % Stearic Acid (B Flake)/5.0 TO 7.0 Loading Levels % Water/40.0 TO 65.0 Loading Levels % Triethanolamine-85%/0.75 TO 1.50 Loading Levels % Pale Oil/0.25 TO 0.50 Loading Levels % |
配制方法: |
Mix Stearic Acid and Pale Oil in mixer. Add 100 gallons of hot water. Heat to 160'F. Start mixer and begin adding half of the Tripoli R-15. Blend in the Triton X-100 and the balance of the hot water (approximately 60% of total water). Add the remaining balance of Tripoli R-15. If temperature is at 160'F and mixture is smooth, mix the Triethanolamine while turning the heat off the mixer. Add a little hot water to help the Triethanolamine mix well. Add the balance of (cold) water to the mixture. Cool mix to 130'F. Pull mixture into drums and let cool. NOTE: Add 5% Dowacide in hot weather to keep down bacteria. |
|