    配方类型: PAPER
    配方说明: Sizing for Blueprint Paper
    配方组成: Sodium hydroxide/1.44 lb
    Water/350 gal
    Preservative (sodium ortho-phenyl phenate)/61.7 lb
    Animal glue/300 lb
    Buffer (borax)/12-27 lb
    配制方法: The sodium hydroxide is dissolved in 250 gal of the water, after which the glue is added and allowed to soak and swell for two hours with brief, intermittent stirring. Then, the solution is steam-cooked at 130' to 140'F to completely disperse the glue. A buffered solution is made with the remaining 100 gal of water and borax. the hot glue dispersion is added to it with stirring, and after thorough mixing the new solution is diluted to the desired Baume. Mixing the two solutions brings the system to about the proper temperature for sizing (90' to 115'F). If desired, 12 lb of a suitable filler can be suspended in the buffered solution. this kind of glue size is not, however, sufficiently resistant to water to permit usage of the paper under conditions of high humidity or actual exposure to water. Therefore, the sized paper is passed through a second solution containing approximately 2% glyoxal, 1% aluminum sulfate, and a small amount of a suitable wetting agent. The paper is dried and, if extreme water resistan

    返回数据库查询
    其他库:化学品法规 国家标准 化学品安全数据库(msds) 外贸常识 合同范本 报关指南 商检指南 国际区号 国家代码