    配方类型: POLISH
    配方说明: Emulsion of "Shanco" W-1119 Wax/Polyethylene
    配方组成: Morpholine/20
    Polyethylene (Emulsifiable)/80
    Water---(208-212'F)/610
    Oleic Acid (Pale)/20
    (Solids 16%)/750 lb
    "Shanco" W-1119 Wax/20 lb
    配制方法: Heat the "Shanco" W-1119 Wax, polyethylene and oleic Acid to a fluid melt at 250'F. Add the morpholine and mix slowly for about 5 minutes.
    Remove open flames before adding the morpholine. Adjust temperature of the base at around 240'F.
    Have the water at 208-210'F, just under boiling and agitate rapidly to produce a vortex. Pour the hot base slowly into the side of the vortex at a rate that will not create boiling. Mix rapidly for 5 minutes. Cool while agitating slowly.